Description
>>> GebrAnw-Dental-Base-Alloy-Adornova-Light.pdf <<<
| Type: | Metal-ceramic alloy on the palladium basis, type 4 (extra hard)
acc. DIN EN ISO 22674 |
| Colour: | white |
| Applicable scope: | Inlays, Onlays | ● |
| Crowns | ● | |
| Small bridges | ● | |
| Middle-sized bridges | ● | |
| Milling, cone and attachment works | ● | |
| Modeling casting | ● |
| Composition: | Pd | 56,00 |
| (mass fraction in %) | Ru | 0,20 |
| Ag | 32,00 | |
| Sn | 8,80 | |
| Ga | 2,00 | |
| In | 1,00 |
| Technical specifications: | Density in g/cm³ | 11,3 |
| Vickers hardness HV 5/30 | (s)260 (n)260 (a-n)280 | |
| Yield strength Rp0,2 in MPa | (s)520 (n)560 (a-n)570 | |
| Elongation at break in % | (s)8 (n)7 (a-n)7 | |
| Average linear CTE 25 – 500 °C in 10-6 K-1 | 14,8 | |
| Average linear CTE 25 – 600 °C in 10-6 K-1 | 15,0 | |
| Elastic modulus in GPa | 130 | |
| Melting interval in °C | 1080 - 1200 |
| Processing: | Preheating temp. of the casting moulds in °C | 900 |
| Casting temperature in °C | 1350 | |
| Crucibles | Ceramic | |
| Curing | 550°C/15min |
| Suitable solders: | Joints before ceramic firing | AL 1060 W |
| Joints after ceramic firing | AL 750 |
1) Brief description:
s – self-curing, n – after ceramic firing, a-s – curing from s condition
a-n – curing from n condition
2) All information about cured condition is given according to the alloy:
– Oxide firing 10min/ 960°C + 4x4min/ 960°C for yellow conventional bonding alloys
– Oxide firing 10min/ 980°C + 4x4min/ 980°C for white conventional bonding alloys
– Oxide firing 10min/ 800°C + 4x4min/ 800°C for LFC-systems
Corresponding data are true under these conditions only.